Surface level documentation on carbon fiber manufacturing. Please reach out to the appropriate mechanical lead or expert to instruct you with more detail before attempting.

 Abbreviations

Carbon Fiber (CF)

All composites work should take place in the composites room and using appropriate PPE

Flat Layups

5 layers of mould release chalk/wax (wipe between each layer application, and let sit after application for ~5 minutes).

Layer epoxy → CF → epoxy → CF … etc. → epoxy → peel ply fabric.

  1. With a disposable brush, paint a layer of epoxy onto the surface of the mold.

  2. Place the CF piece.

  3. Paint a layer of resin on top of the CF piece.

    1. Make sure to do shorter brush strokes + more stippling rather than long strokes. Long strokes increases the risk of the CF strands getting caught in the brush. The goal is to push resin into the CF and long stroke won’t help achieve this.

  4. Squeegee out excess resin.

  5. Repeat steps 2-4 per each layer.

  6. After all the layers are done, place the peel ply fabric on top of the final layer.

  7. Press the peel ply fabric to make sure that it absorbs excess resin from the final layer. A squeegee will help achieve this effect.

  8. After the resin has cured, you can tear the peel ply off (it should come off pretty nicely). Use a scrapper or a blade to release the wet layup from the mold.

General rule is weight of carbon fiber == weight of epoxy resin solution. Do not forget to tare (or subtract) the weight of the cup that holds the resin.

Aeropoxy epoxy resin solution = 100 parts epoxy, 27 parts hardener (the ratio might differ depending on the hardener and resin used so make sure to read the container label).

Other notes:

  • Bends and complex curves have a higher chance of introducing air bubbles which will stop the epoxy from flowing into that particular area. This leads to small dents/holes/dry spots after the epoxy cures. Air bubbles are almost unavoidable because air particles will enter the resin when you are mixing it with the hardener.

    • To minimize air bubbles you can:

      • de-gas your resin using a vacuum chamber

      • let the epoxy mixture sit for longer after mixing (but you will need a longer epoxy pot life)